How Thick Should Copper Plating Be in a Plated Hole?

For Class 3 work the barrel needs 25 micrometres of copper on average and never less than 20 at any single point. Class 2 drops those numbers to 20 and 18. The average is what the inspection certificate quotes; the thin point is what decides whether the joint survives thermal cycling, so the second number belongs on the drawing.

Both figures come from IPC-6012, Table 3-10, and both are measured on a microsection, never on the surface. Surface copper says nothing about the barrel: a board can carry 35 micrometres of foil on the outer layer and 15 micrometres at the middle of a 0.30 mm hole on the same panel.

Why the middle of the barrel is always the thin end

Plating happens in a tank, and the electrolyte has to reach the middle of the hole before copper can deposit there. In a 0.30 mm hole through a 1.6 mm board, the middle sits 0.8 mm from either opening and the solution in that region is refreshed by diffusion rather than by flow. Current density follows the same geometry: it peaks at the two rims and bottoms out at the centre, so copper builds where it is not needed and starves where it is.

The ratio that governs the effect is depth divided by diameter, the aspect ratio. Our standard FR-4 line is rated to 10:1, which on a 1.6 mm board sets a 0.16 mm floor on drill diameter, and the high layer count line goes to 25:1. At 25:1 the middle of the barrel sees very little exchange, and the difference between the rim reading and the centre reading stops being noise. That is the whole reason Class 3 names a thin-point limit instead of trusting an average of four measurements.

Plating also narrows the hole. Twenty five micrometres per side takes a 0.30 mm drill down to a finished 0.25 mm, and a 0.20 mm drill down to 0.15 mm. A drawing that asks for a 0.30 mm finished hole with Class 3 plating therefore needs a 0.35 mm drill, which is a different tool, a different aspect ratio and sometimes a different price.

The electrical consequence is small but not zero. A 1.6 mm long barrel of 0.30 mm diameter measures about 1.17 milliohms at 25 micrometres of wall and 1.46 milliohms at 20, so a via carrying 3 A drops 3.5 mV against 4.4 mV. At that diameter thickness is a mechanical argument rather than an electrical one. It turns electrical when the hole shrinks: the same 1.6 mm barrel at 0.20 mm diameter reads 1.75 milliohms at 25 micrometres and 2.19 at 20.

When thickness stops being the answer

A thicker barrel resists thermal strain better, and the strain is real. Between room temperature and reflow peak a 1.6 mm FR-4 board grows roughly 20 to 35 micrometres in Z, while the copper barrel grows about 6. The laminate therefore pulls the barrel into tension twice per reflow, and the copper has to stretch without cracking. Electrodeposited copper with columnar grain structure stretches less before it breaks than fine grain copper, which is why ductility is quoted alongside thickness in high reliability work and why a 25 micrometre barrel from a badly controlled bath can fail where a 20 micrometre barrel from a good one survives.

Going thicker has a cost at the other end. Every extra micrometre of wall closes the hole, reduces the annular ring left after drill registration, and lengthens plating time, which worsens the rim to centre spread that the exercise was meant to fix. A 50 micrometre barrel in a 0.20 mm hole leaves a 0.10 mm finished hole, and no probe, pin or reflowed lead is going into that.

Voids behave differently from thin spots. A thin wall is a gradual weakness; a void is a stress riser and a path for plating solution to sit in after the fact. Class 3 allows none in the barrel, Class 2 allows limited ones, and both are read on the same section as the thickness.

Three ways the requirement gets lost

Writing the average only. "25 micrometres minimum" on a purchase order is read by most shops as an average target, and a barrel that reads 25 at the rim and 18 in the centre passes the sentence and fails the class. Write both numbers: average and thin point.

Sectioning near the opening. A microsection cut close to the entry shows a healthy wall because the entry is where the copper is thickest. The measurement has to be taken at the centre of the barrel, on the hole that is actually the deepest or the smallest on the panel, not on the most convenient one.

Asking for Class 3 copper and nothing else. Class 3 is a package: 50 micrometres of external annular ring with no breakout, 25 micrometres on the internal ring, no barrel voids, and tighter drill registration than Class 2. A stack that keeps Class 2 pads with Class 3 plating produces a board that fails on the ring before anyone measures the wall. The ring arithmetic sits in minimum annular ring for a plated hole.

What SUPERB PCB holds

Published figures: plating 20 micrometres and above, mechanical drilling 0.15 to 6.35 mm, laser drilling 0.075 to 0.15 mm with 0.05 mm available, aspect ratio 10:1 on the standard FR-4 line and up to 25:1 on the high layer count line, hole position plus or minus 0.075 mm, plated hole size plus or minus 0.075 mm and plus or minus 0.05 mm for press-fit, board thickness 0.6 to 3.2 mm, 1 to 20 layers standard and up to 68 on the high count line. Cross-section and impedance reports ship as standard, and a first article section is taken before the panel is released. The same figures sit on the FR-4 process parameters page and on the capability page.

Where the honest boundary sits: 20 micrometres is what the line guarantees, and a Class 3 order is quoted with 25 micrometres as the working target because the thin point has to clear 20 after etchback and sectioning. If a drawing asks for 30 micrometres average at 25:1 aspect ratio, we say so before the panel starts rather than after the section. For medical and defense builds the plating, the section and the void count are reviewed together, which is the same discipline the high reliability PCB work runs on.

What to send with the drawing

The IPC class with its revision, the average and the thin-point minimum, whether the hole is a via or a component hole, the finished hole size against the drill size you expect, the maximum aspect ratio on the stack, the current the via will carry, the thermal cycling the assembly has to pass, and whether cap plating is required over a filled via, which is 12 micrometres at Class 3 against 5 at Class 2. Those eight lines settle the plating before the first panel, which is the only moment when changing it costs nothing.