A 1.6 mm FR-4 board grows 0.05 to 0.08 mm through a lead-free reflow, which is 3 to 5 percent of its thickness. About 90 percent of that growth happens above Tg, in the last 90 °C of the profile.

That fraction of a millimetre is the whole reason a plated barrel survives or cracks. The copper wall has to stretch with the laminate, and the laminate expands three to five times faster per degree once the resin softens. Anyone who specifies Tg and stops there has half the number.

What the CTE numbers actually are

Below Tg the z-axis CTE of FR-4 is 50 to 70 ppm/K. Above Tg it is 200 to 300 ppm/K. In the plane the CTE is 14 to 17 ppm/K and it does not step at Tg, while copper is about 17 ppm/K, which is why a plated hole in the plane is nearly stress free and a plated hole through the thickness is not.

Total z-axis expansion from 50 to 260 °C is 2.5 to 4.5 percent for standard grades, measured by TMA to IPC-TM-650 2.4.24 on a 1.6 mm specimen. Standard Tg 130 to 140 laminates sit at the top of that range, high Tg 170 to 180 laminates at the bottom. Both are FR-4, and both are sold as FR-4 on a purchase order that names no grade.

What it does to a real board

The expansion is proportional to thickness, so the same material on a thicker board pulls the barrel further. At 4 percent total expansion:

Board thicknessGrowth at 4%Strain on the barrel
0.8 mm0.032 mm4%
1.6 mm0.064 mm4%
2.4 mm0.096 mm4%
3.2 mm0.128 mm4%

The percentage stays the same because the barrel is as long as the board is thick. What changes is the absolute movement: 128 µm at 3.2 mm against 32 µm at 0.8 mm. A thin board is not safer, it is the same strain over a shorter wall, and a thin wall work hardens faster.

The strain has to be compared with what plated copper can take. A 20 to 25 µm electroplated wall has finite elongation, and a 4 percent stretch already uses most of it, which is why a 1.6 mm standard Tg board is at the edge of a 1,000 cycle thermal test rather than in the middle of it. A thicker plating helps, and so does a laminate that expands less.

Tg is the main lever, and it is not the only one

Because most of the expansion happens above Tg, moving Tg up 40 °C removes one to two points of total growth. A Tg 130 grade reaches 260 °C at 130 degrees above its transition and expands 4 to 5 percent. A Tg 170 grade does the same trip at 90 degrees above and expands 2.8 to 3.5 percent. A Tg 200 grade lands near 2.5 to 3 percent.

Td and T288 matter too, for a different failure. Td is the 5 percent weight loss point by TGA, 310 to 320 °C for a standard grade and 340 to 360 °C for a high Tg one, and T288 is the minutes the laminate survives at 288 °C before it delaminates. A standard grade at 2 minutes survives the first reflow and not the third rework. A high Tg grade at 20 to 30 minutes does.

Three mistakes that show up on the cross-section

Specifying Tg and nothing else. Two Tg 170 laminates can differ by a full point in total expansion, and by 10 minutes in T288. If the drawing says FR-4, Tg 170, the shop is free to pick the cheapest sheet that meets both numbers, and that sheet may be the one at 4 percent.

Using a standard Tg on a 2.4 mm or 3.2 mm board because the stackup has few layers. Thickness drives expansion, not layer count. A 3.2 mm standard Tg board moves 128 µm at reflow, and the plating that has to absorb it is the same 25 µm as on a 1.6 mm board, with an aspect ratio that is now harder to plate evenly.

Ignoring moisture. FR-4 takes up 0.1 to 0.2 percent moisture in storage, and that water flashes to steam above 100 °C. The steam adds internal pressure on top of the CTE strain and it is the usual trigger for delamination and measling after reflow. Baking to J-STD-033 before the first reflow removes the variable, and it costs a day of schedule if it is remembered at the end instead of the start.

How we hold the number

SUPERB PCB stocks Tg 130, 150 and 170 grades from Shengyi and Kingboard, with the grade named on the traveller rather than on the drawing only. Standard thickness is 0.6 to 3.2 mm with a tolerance of ±0.10 mm under 1.0 mm and ±10 percent above, extended capability runs 0.1 to 12 mm, plated copper is 20 µm or more, and the aspect ratio is held at 10:1 on the standard line and up to 25:1 on the high layer count line, which runs to 68 layers.

Every lot gets a cross-section report on 10 holes, and the panels that go to assembly are baked to J-STD-033 before the first reflow. If the drawing calls for a 1,000 cycle thermal test, the laminate grade is chosen for it at quoting, not after the first lot fails. The material options are on the FR-4 process parameters page, the thickness and aspect limits in PCB capability, and the reliability side in high reliability PCB.

Next step

Send the stackup, the board thickness and the thermal test you have to pass. We will name the laminate grade that holds the expansion under your limit, quote it, and state the plating thickness and aspect ratio the build will carry, so the CTE question is answered before the first panel is laminated.