A bridge is found at electrical test, usually at the last station, and by then the board has been through the oven, the wash and the coat. It is scrapped or reworked, and the report says bridging, which tells the next person nothing about the cause. In most cases the cause was at the printer, two processes and one oven earlier.
Solder bridging prevention comes down to keeping two pads apart until the alloy freezes. Everything that closes that gap early is either paste in the wrong place, a stencil that did not seal, a mask dam too thin to hold, or heat that arrived unevenly.
What actually forms a bridge
Paste is printed, the part lands, and the oven melts the alloy. While it is liquid, surface tension pulls a joint toward its own pad, and the same force pulls two nearby joints toward each other if the volume is high enough to touch. A bridge is therefore a volume problem first and a spacing problem second.
Three things make it worse: too much paste, paste that slumps before reflow, and a mask dam narrow enough that the alloy wets straight across it. Flux behaviour sits behind all three, because what holds the alloy on its pad is the surface energy the flux leaves behind.
The printer sets the volume
A stencil aperture releases paste in proportion to its area and its walls. When the aperture is small compared with the stencil thickness, paste sticks to the walls instead of transferring, and the printer compensates with pressure. Pressure then pushes paste under the stencil onto the mask between pads, which is a bridge that appears only after reflow.
Area ratio is the number to hold: aperture area divided by wall area. Below the working limit, the deposit is inconsistent, and inconsistent deposits on a 0.5 mm pitch part are exactly where bridges cluster. The full set of thickness and ratio figures is on the stencil thickness and area ratio page.
Where bridges are born, by symptom
| What the board shows | What caused it | What to change |
|---|---|---|
| Bridges between the same two pads on every board | Aperture too large or walls damaged on that opening | Re-cut the aperture to the pad, inspect the stencil under light |
| Bridges on one end of the panel only | Stencil not sealed at that end, or the panel is not flat | Check support pins and squeegee pressure balance |
| Bridges after a paste change | New paste slumps in the pause between print and reflow | Shorten the wait, adjust the profile, or change the pause handling |
| Bridges under a connector or shield frame | Paste pushed into a cavity and reflowed with nowhere to go | Reduce the deposit, add a mask dam, vent the cavity |
| Bridges on the wave side only | Flux not driven off in preheat, drag across adjacent pads | Raise preheat, change the drag angle and the pallet |
| Bridges that come and go between lots | Mask dam width at the process limit, wetting across on some boards | Widen the dam, or split the pad with mask |
What holds two pads apart
The mask dam between pads is the last barrier before the alloy touches. We hold a dam width of 3.5 mil on green mask, 5 mil on white and black, 4 mil on the other colours, and 50 µm on HDI, because a dam that survives one board and breaks on the next turns a controlled process into a lottery. Where a dam cannot be wide enough, the answer is a different pad geometry, not a tighter print.
Inside the laminate the same discipline applies at a smaller scale: our fine line work runs to 0.05 mm line and space, and BGA pads at 10 mil on HASL or 8 mil on ENIG, with 0.45 mm pitch on standard boards and 0.30 mm on HDI. These numbers decide how much room is left for paste to spread before two joints meet.
Reflow, and the part of it people skip
A profile that heats the board unevenly melts one side of a part before the other. The first joint to melt wets and pulls; the second is still solid paste. That difference is how a bridge forms on a part that printed correctly. We run a twelve zone oven with SAC305 and nitrogen below 500 ppm, and the profile is verified on the board rather than on the oven display.
The verification method is on the reflow profile verification page. What matters for bridging is the soak: too short, and the flux does not drive off before the alloy flows.
Wave and selective solder are a different failure
On a wave, a bridge is a peel problem. Solder leaves the joint as the board lifts, and if the flux is spent or the preheat is low, the alloy does not release cleanly from between two pins. Pin length, pallet opening, drag speed and the direction of travel all move the result, and so does the gap between the pad and the hole.
Selective solder narrows the same physics to one nozzle. A nozzle that delivers more than the joint can take floods the neighbouring pin. The process notes are on the selective soldering process page.
How SUPERB PCBA catches it before test
The deposit is measured at the printer with 3D SPI, so a bridge that would only appear at reflow is caught as a volume outlier before the part is placed. After reflow, optical inspection reads the joints, and X-ray takes the ones under a package. Seven SMT lines run the first article on the machine that will build the order, and that first panel is checked against the same limits that will be used for the last one.
The measurement side is covered in solder paste inspection. Where a board arrives with pads too close for the process, the conflict is raised before tooling, because a pad change after a stencil is cut costs more than the stencil.
Questions buyers ask
Is a bridge always a printing problem?
Mostly, but not always. A mask dam at its limit, a profile with a short soak, or a part that warps at reflow will bridge on a perfect print.
Can bridging be quoted as a defect rate?
No. It depends on pitch, pad geometry, paste and part mix. What can be stated is the process and the measurement behind it.
Does nitrogen remove the problem?
No. Nitrogen improves wetting, and better wetting can pull alloy further along a mask surface if the dam is thin.
Next step
Send the Gerber set, the BOM and the panel drawing. The print and mask review comes back with the apertures that need changing and the pads where a dam cannot be held, before a stencil is cut.