The board passes every station. Optical inspection sees a ball array, X-ray sees round balls, electrical test passes. Six months later a unit comes back with an intermittent fault that will not repeat on the bench, and a cross section shows the ball resting on the paste instead of being joined to it.
That is a head in pillow defect: the solder ball and the printed paste both melted, but they never merged. The ball sits on top of a collapsed deposit like a head on a pillow, in contact but not bonded, and the joint holds until vibration, thermal cycling or a drop opens it.
What has to happen for the two to meet
During reflow, the paste under a ball melts first and pulls itself up by surface tension while the ball is still solid or partly solid. If the ball is also moving away, because the package is warping as it heats, the two surfaces oxidise in the gap and never touch again. The alloy freezes with a boundary instead of a grain structure across it.
So a head in pillow joint needs two conditions at once: a package that lifts at the moment the paste is liquid, and a paste deposit that does not have the volume or the activity to reach it anyway.
Warpage is the usual root cause
A plastic package is not flat at reflow temperature. The substrate and the mould compound expand at different rates, and the ball side can go concave or convex depending on the package, the moisture content and the ramp. The moment of maximum warp is often within a few seconds of the paste going liquid, which is exactly the window where the joint is supposed to form.
Moisture makes it worse. Parts that absorbed water during storage release it at reflow and the package moves further. Handling and baking are covered on the moisture sensitivity and bake control page, and the package level limits sit in the J-STD-020 and J-STD-033 tables we work to. Bake at 125 °C before the run is cheap; a field return is not.
Signals, causes and what to change
| What the data shows | What caused it | What to change |
|---|---|---|
| Open appears only after thermal cycling | Ball touching paste, no bond across the boundary | Treat as a reflow and warpage problem, not a handling problem |
| Same package position fails across lots | Package warp at peak temperature | Lengthen the time above liquidus, lower the peak, or support the package |
| Failures after a storage gap | Moisture absorbed before the run | Bake to the floor life limit, keep dry pack intact |
| Failures on the thin package only | Deposit too small to bridge the warped gap | Increase paste volume within the aperture limit, check the stencil step |
| Joints look dull at the boundary | Oxidation during a long soak | Shorten the soak, review the nitrogen level |
| Mixed alloy on the same board | Leaded paste against lead free balls | Check the alloy pairing before the build |
Why the line does not catch it
Optical inspection reads the surface, and the surface of a head in pillow joint is a row of balls. A 2D X-ray reads density, and the ball is dense, so a gap of twenty or thirty microns under it disappears into the ball's own shadow. Electrical test passes because the two surfaces are in contact when the board is cold and flat.
What does catch it is either a cross section, a dye and pry check, or computed tomography at a resolution fine enough to show the boundary. None of these run on every board. The practical answer is to remove the conditions rather than to inspect for the result, and to use the inspection on the first article and on any change of package, paste or profile.
The alloy pairing
Mixing a leaded paste with lead free balls lowers the melting point of the paste and raises the melting point of the ball, and the difference is enough to produce the same non-merge. The physics and the permitted combinations are on the mixed alloy page. Where a legacy board has to keep a leaded process, the ball alloy has to match it.
How SUPERB PCBA holds the window
The profile is measured on the board, not read off the oven display: twelve zones, SAC305, nitrogen below 500 ppm, and a thermocouple on the package that matters. Packages are baked to the floor life limit before the run, and the dry pack is opened against the plan rather than against convenience.
For the joints that cannot be seen, X-ray View-x1800 runs in 2D or CT, and void and boundary checks follow IPC-7095. Bare boards are held to 0.75 per cent warpage for the assembly side, because a board that is not flat changes the gap under every ball on it. The profile side is on the reflow profile verification page, and the X-ray station on the 2D and CT inspection page.
Seven SMT lines run the first article on the machine that will build the order, so a package that warps out of the window is found on one panel rather than in a field return.
Questions buyers ask
Can a head in pillow joint be prevented on every package?
Not every package, but the window can be held for the packages that are known to warp. The work is profile, bake and deposit, in that order.
Does a longer time above liquidus always help?
Up to a point. It lets the ball settle into the paste, and past that point it grows the intermetallic layer and damages nearby parts.
Is 2D X-ray enough?
No. It sees voids and missing balls well, and a boundary under a ball is not a void.
Next step
Send the BOM, the Gerber set and the package list, with any part that has given this fault before marked. The reflow window and the bake requirement come back per package, before the first panel runs.