A backplane passes flying probe, then fails in circuit test after two reflow passes. The cross section shows 16 micrometres of copper at the middle of a 3.2 mm deep via against a 20 micrometre floor. Surface copper measured well inside tolerance. Only the barrel was thin, and nothing on the incoming report had asked about it.
Plating thickness is what decides whether a via survives assembly and thermal cycling, and it is read in three places that are usually quoted as one number.
Three thicknesses that share one name
Hole wall copper is the metal deposited inside a drilled hole. It carries current between layers and it is the thinnest copper anywhere on the board, because deposition inside a hole depends on electrolyte reaching the middle of the barrel.
Surface copper is the foil plus the plating on the outer layers. It sets trace resistance, current capacity and the etch profile, and it is what most buyers mean when they say 1 oz or 2 oz.
Finish metal sits on top of the copper. Nickel and gold on ENIG, tin on immersion tin, solder on HASL. It protects the copper and provides a solderable or bondable surface, and it adds no current carrying capacity worth counting.
A report that gives one figure without saying which of the three it measured cannot be checked against a drawing. Ask for the barrel, because that is where the failures are.
Where the barrel goes thin
Plating inside a hole is a race between chemistry and geometry. Electrolyte has to reach the middle of the barrel and fresh ions have to leave, so copper at mid hole is always thinner than at the entry and exit. The wider that gap, the worse the throwing power.
Aspect ratio is the main lever, depth divided by diameter. A 3.2 mm board with a 0.3 mm hole is 10.7 to 1, and the middle of that barrel sits far from the surface. Builds up to 25 to 1 need slower plating, more agitation and a longer cycle, so they belong on a line set up for them.
Hole size works the other way. Drilling covers 0.15 to 6.35 mm, laser drilling 0.075 to 0.15 mm with 0.05 mm available. Small holes plate more evenly but are harder to clean; large holes clean easily but starve in the middle when the board is thick.
Copper distribution across the panel decides current density at each hole. A panel with a large ground plane on one side and sparse routing on the other plates unevenly, and the sparse area takes more current per unit area. That is the same imbalance that shows up as bow and twist, covered under copper balance.
Drill quality decides whether the copper sticks. Smear, glass fibres pulled out of the resin or a rough barrel wall leaves a thin spot that no plating cycle can fill, and the void shows up later as an open.
The numbers that hold on a lot
| Parameter | Working value | Where it is read |
|---|---|---|
| Hole wall copper | 20 micrometres minimum | Cross section of the plating coupon, three points per barrel |
| Inner layer base copper | 0.5 to 4 oz | Laminate specification, checked on the incoming sheet |
| Outer layer copper, standard | 1 oz | Surface measurement after plating |
| Outer layer copper, maximum | 6 oz inner, 10 oz outer | Agreed per stack up before the panel is released |
| ENIG nickel | 100 to 200 micro inches | XRF on the pad, cross section on the coupon |
| ENIG gold | 2 to 3 micro inches | XRF on the pad |
| Aspect ratio | 10 to 1 standard, 25 to 1 on the high layer line | Stack up, checked before drilling |
| Plated through hole diameter | Plus or minus 0.075 mm, plus or minus 0.05 mm on press fit | Pin gauge, cross section |
| Annular ring after plating | 3.5 mil on vias at 1 oz, 8 mil on component holes | Cross section, X-ray of the coupon |
Two of those rows are floors, not targets. A lot that averages 24 micrometres with one barrel at 18 fails, so the thinnest reading on the barrel is the one that goes on the report.
How the value is proven
Plating thickness is read on a coupon built into the panel border, not on the product. The coupon carries the same hole sizes and the same aspect ratio as the densest area of the board, so the reading means something. It is cross sectioned, polished and measured at the entry, middle and exit of at least three barrels, and the lowest figure is the one reported.
Surface copper and the finish metal are read by XRF on the finished pad. Where a drawing names a method the report follows it, and each result carries a microsection photograph so the number traces to a feature a buyer can see.
What SUPERB PCBA works to
Boards are built to print from the Gerber, stack up and drill file supplied. The published envelope covers 1 to 20 layers on the FR-4 line and up to 68 layers on the high layer line, HDI at 1 to 3 stages, finished thickness 0.6 to 3.2 mm standard and up to 12 mm extended. Barrel copper is held at 20 micrometres or more and is quoted the same way on every lot. The full table sits on the PCB capability page.
Heavy copper is available to 6 oz inner and 10 oz outer, and it changes the etch and the solder profile long before it changes the plating, which is covered under when 4 oz copper changes the etch and solder profile. Where a build needs a small hole in a thick board, the limit is aspect ratio rather than the drill bit, covered under how small a hole can be drilled in a thick board.
What to send with the enquiry
- Gerber and drill file, with plated and non plated holes separated.
- Stack up with base copper weight per layer, prepreg type and finished thickness.
- The barrel copper you need, and whether the figure is a minimum or an average.
- The finish and its thickness, plus any hole that has to be press fit.
Questions buyers ask
Is 20 micrometres a minimum or an average?
It is a minimum, read at the thinnest point of the barrel, which is normally mid hole. A process that holds 20 as an average will produce barrels under it, and those are the ones that crack in thermal cycling.
Can heavy copper and a small hole be combined?
Only inside the aspect ratio. A 4 oz inner layer on a 3.2 mm board limits the finished hole that can be plated, and the drill table gives the number for that thickness. Send both and the pair is checked before quoting rather than after the first panel.
Next step
Send the stack up with base copper per layer, the drill file and the barrel copper you need. SUPERB PCBA returns the plating window for that build, the hole sizes it will hold at that thickness and the coupon plan for the lot, so the thickness is agreed before the first panel is plated.