Contact Us
  • Home
  • BLOG
  • How Much Gold Makes a Solder Joint Brittle?

How Much Gold Makes a Solder Joint Brittle?

Above 3 percent gold by weight in the joint. That is the limit J-STD-001 sets for tin lead solder, and it is the number that turns a cosmetic gold surface into a brittle joint. In lead free SAC305 the threshold is higher, around 10 percent, but the same mechanism applies: gold dissolves into the molten solder, forms gold tin intermetallic, and the joint loses ductility where the load is highest.

The useful question is not how thick the plating is in microns. It is how much gold ends up in a given volume of solder, which is why a 1 micron finish on a small pad is more dangerous than a 1 micron finish on a large one.

The arithmetic that decides it

Gold has a density of 19.3 grams per cubic centimetre, so 0.1 micron of gold weighs 1.93 micrograms per square millimetre. A 0.5 by 0.5 mm pad, 0.25 square mm, carries 0.48 micrograms at that thickness. A joint on that pad measuring 0.4 by 0.4 mm with a 0.1 mm standoff holds 0.016 cubic mm of SAC305, which at 7.4 grams per cubic centimetre weighs about 118 micrograms. The gold is 0.4 percent of the joint, harmless.

Change the finish to 1 micron of hard gold, the thickness used on edge connectors, and the same pad carries 4.8 micrograms, which is 4.1 percent of the joint weight. That is above the tin lead limit and well into the brittle range. Two microns on a 1 square mm connector pad with a 0.15 mm joint reaches about 3.5 percent, and on a smaller joint the same thickness goes past 8 percent.

This is why an immersion gold thickness of 0.05 to 0.1 micron works and a hard gold finger never does. The finish is not better because there is more gold. It is only more gold.

What the gold does inside the joint

Gold dissolves quickly in molten tin. At reflow the plating disappears into the solder within seconds, and on cooling it precipitates as AuSn4 platelets and needles, or as (Au,Ni)Sn4 where the nickel from an ENIG deposit is present. Those phases are hard and brittle, they sit at the interface where the thermal expansion mismatch is already concentrated, and they coarsen with every additional reflow. A joint that survives one pass can crack after the second.

Two details make it worse. Gold dissolution is faster in lead free solder than in eutectic tin lead, and slower cooling gives the intermetallic more time to grow into large plates. A large plate at the fillet root is a crack waiting for the first thermal cycle, and the failure looks like a joint that simply fell off at low load.

Where the mistake usually sits

Specifying hard gold on pads that will be soldered because gold sounds like the premium finish. Hard gold contains cobalt or nickel to resist wear, it is 0.8 to 2 microns thick for connector life, and it is meant for sliding contacts only. On a solderable pad it is a brittle joint in waiting. Edge fingers stay hard gold, the pads next to them should not.

Checking thickness with X ray fluorescence and stopping there. XRF gives microns on the surface and says nothing about the joint volume or the number of reflows that pad will see. A 0.15 micron reading on a 0.2 square mm pad is a different risk from the same reading on a 2 square mm pad.

Reworking on the same gold without removing the old solder. The second melt dissolves what is left of the plating into a smaller joint, and the gold percentage goes up. Thick gold needs the solder removed and the surface wicked before the joint is remade.

Forgetting the second reflow. A board with parts on both sides sends the same joint through two melts. If the finish was already at the edge of the limit, the second pass pushes it over.

How to keep gold out of the danger zone

Use immersion gold at 0.05 to 0.1 micron on solderable pads, ENIG or ENEPIG, and keep the nickel barrier under it. Check thickness by XRF per panel and log the reading against the lot. Where the drawing asks for thick gold on a solderable area, remove it by wicking with hot solder before assembly, twice where the plating is above 1 micron. Choose immersion tin or a solder levelled finish for pads that only need to be soldered, and keep hard gold for the contacts that slide. If a joint has to be reworked, remove the solder first, then remake it, and do not reuse the gold surface as if it were fresh.

On the inspection side, gold embrittlement does not show as a void. It shows as a crack at the interface after thermal cycling, with a flat fracture face and little deformation. Cross sections plus energy dispersive analysis on the fracture face will show the gold, and that is the report a customer will ask for when a joint fails at low mechanical load.

How we build it

Surface finish on a SUPERB build is fixed against the drawing, not by habit. ENIG is held at 0.05 to 0.1 micron immersion gold over 3 to 6 microns of nickel, checked by XRF and recorded per lot. Where a customer drawing calls for thicker gold on a solderable pad, the gold is wicked before the first print and the rework is documented. Hard gold stays on edge contacts. The finish options are listed in PCB capability, the reliability build options in high reliability PCB, and the incoming checks in PCBA quality standards.

SUPERB PCB and SUPERB Tech also quote the finish with the assembly, so the plating and the reflow count are decided together instead of on separate purchase orders.

Next step

Send the drawing with the finish callout, the gold thickness and the number of reflow passes the assembly will see. We will come back with the finish that keeps the joint under 3 percent gold, and the checks that prove it on the first lot.

Need the finish checked against your drawing? pcba@superb-tech.com · WhatsApp +86 133 9608 1443