A 240 piece backplane lot passes flying probe, then eleven boards fail at functional test. The cross sections come from the same panel: 27 micrometres of copper at the barrel nearest the rack contact, 18 micrometres in the middle of a barrel at the far edge. The average was inside the floor. The spread was not.
Plating uniformity is the part of copper control that a single figure hides. It decides yield on thick boards, on heavy copper and on any build with a wide difference in pattern density.
Three spreads behind one figure
Across the panel: copper near the contact point sees a shorter current path than copper at the opposite edge, so the same panel can plate at two rates. On a 622 by 1092 mm panel the difference is measurable even on a well set line.
Through the barrel: electrolyte has to reach the middle of the hole and fresh ions have to leave. Entry and exit always plate heavier than mid hole, so a barrel that reads 30 micrometres at the surface can be at 20 in the middle.
Hole to hole: a sparse area draws more current per unit area than a dense one, so isolated holes plate heavier than holes inside a ground plane. That is the same imbalance that shows up later as bow and twist.
A report that gives the lot average cannot be checked against a drawing, because the number that decides survival is the thinnest point on the worst barrel, not the mean.
What the spread is read against
| What is compared | Value the lot holds | Where it is read |
|---|---|---|
| Thinnest barrel in the lot | 20 micrometres minimum | Cross section at entry, middle and exit of three barrels |
| Barrel at rack contact against barrel at panel edge | The lowest reading is the one reported | Coupon set placed at both positions on the panel |
| Surface copper in dense and sparse areas | 1 oz standard outside, 0.5 to 4 oz base inside | XRF on pads in both areas after plating |
| Hole to hole after plating | Plus or minus 0.075 mm, plus or minus 0.05 mm on press fit | Pin gauge on twenty holes spread across the panel |
| Annular ring after plating | 3.5 mil on vias at 1 oz, 8 mil on component holes | Cross section, X-ray of the coupon |
| Aspect ratio the line plates evenly | 10 to 1 standard, 25 to 1 on the high layer line | Stack up, checked before drilling |
| Heavy copper ceiling | 6 oz inner, 10 oz outer, agreed per stack up | Surface reading, cross section on the coupon |
| Panel that keeps current density even | Up to 622 by 1092 mm, one panel per rack position | Panel drawing before release |
The first two rows are the ones a buyer should ask for in writing. A lot at 24 micrometres average with one barrel at 18 fails, and the thin barrel is what opens in the field.
Balancing a panel before it is plated
Copper balance is decided on the panel, not on the plating line. Where one half of the panel is a ground plane and the other is sparse routing, the sparse half plates heavier and etches differently. Adding dummy copper, moving the part within the panel and grouping boards of similar density all reduce the spread before a single panel reaches the line.
The coupon sits in the panel border and carries the same hole sizes and the same aspect ratio as the densest area of the product. It is the only place where a cross section means something, because a section through the product destroys a board.
Rack contact position is the second lever. A single contact at one corner gives that corner a shorter current path; multiple contacts and a symmetric rack arrangement even it out. The same logic is covered from the warpage side under copper balance.
Where the spread is lost after plating
Drilling comes first. Smear, resin pull out or a rough barrel wall leaves a thin spot that no plating cycle fills. Hole position held to plus or minus 0.075 mm keeps the barrel inside its pad, and that is checked against the same datum as the drill file, which is the subject of drill registration.
Etch comes second. Heavy plating etches back further, so a panel that plated unevenly ends with different trace widths in the two areas. Line width is held to plus or minus 20 percent, and on a 0.05 mm trace that allowance is used up quickly.
What SUPERB PCBA works to
Boards are built to print from the supplied Gerber, stack up and mechanical drawing. The published envelope covers 1 to 20 layers on the FR-4 line, up to 68 layers on the high layer line and HDI at 1 to 3 stages, with finished thickness from 0.6 to 3.2 mm standard and 0.1 to 12 mm on the extended range. Hole wall copper is held at 20 micrometres minimum, inner layer base copper from 0.5 to 4 oz, outer layer 1 oz standard with 6 oz inner and 10 oz outer available per stack up. Mechanical drilling covers 0.15 to 6.35 mm and laser drilling 0.075 to 0.15 mm with 0.05 mm available. Plated through holes are held to plus or minus 0.075 mm, 0.05 mm on press fit, and annular ring from 3.5 mil on vias to 8 mil on component holes. Panels run up to 622 by 1092 mm. Standard shipment includes a cross section report, so the thinnest barrel is on paper rather than assumed. The full table sits on the PCB capability page.
What to send with the enquiry
- The stack up with copper weight per layer and the finished board thickness with its tolerance.
- Hole list with finished diameter, plated or non plated, and any press fit position.
- Where the board sits in the panel, or the panel drawing if you supply one.
- The report you need at shipment: cross section only, or cross section with a nine point thickness map.
Questions buyers ask
Is 20 micrometres the average or the minimum?
It is the minimum at the thinnest point of the worst barrel sampled. A lot that averages 24 micrometres with one barrel at 18 does not meet it, which is why the report gives the low reading and the position it came from.
Why does the middle of the barrel come out thin?
Because electrolyte exchange slows as the hole gets deeper relative to its diameter. At 10 to 1 the middle is reachable with normal agitation; at 25 to 1 the cycle has to be slower and the flow stronger, and that work belongs on the high layer line.
Does heavy copper plate as evenly as 1 oz?
No. Longer plating time widens the difference between dense and sparse areas, so heavy copper panels are balanced more carefully and the coupon positions are chosen before release, not after.